{"id":3167,"date":"2023-11-29T10:28:44","date_gmt":"2023-11-29T02:28:44","guid":{"rendered":"https:\/\/www.naxauam.com\/?post_type=docs&#038;p=3167"},"modified":"2025-04-23T16:01:30","modified_gmt":"2025-04-23T08:01:30","password":"","slug":"\ud2f0\ud0c0\ub284-\uc808\uc0ad-\uacf5\uad6c\uc758-hipims-tib2-\ucf54\ud305","status":"publish","type":"docs","link":"https:\/\/www.naxauam.com\/ko\/\ubb38\uc11c\/\ud2f0\ud0c0\ub284-\uc808\uc0ad-\uacf5\uad6c\uc758-hipims-tib2-\ucf54\ud305\/","title":{"rendered":"\ud2f0\ud0c0\ub284 \ud569\uae08 \uc808\uc0ad \uacf5\uad6c\uc758 Hipims TiB2 \ucf54\ud305"},"content":{"rendered":"<h2 class=\"wp-block-heading\">TiB2(\uc774\uc0b0\ud654\ud2f0\ud0c0\ub284) \ucf54\ud305<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Nasi TiB2(\uc774\ubd95\ud654 \ud2f0\ud0c0\ub284) \ucf54\ud305, 3000 HV \uacbd\ub3c4, HiPiMS\ub85c \uc81c\uc870, \ub0ae\uc740 \uc751\ub825 \ubc0f \ub192\uc740 \uce69\ud551 \uc800\ud56d\uc131. \ud2b9\ud788 \ub0b4\ub9c8\ubaa8\uc131 \ubc0f \ub0b4\uae08\uc18d\uc131 \uace0\uc628 \ubd80\uc2dd \uc870\uac74\uc5d0\uc11c \ube44\ucca0\uae08\uc18d(\uc608: \uc54c\ub8e8\ubbf8\ub284, \uad6c\ub9ac, \ub9c8\uadf8\ub124\uc298 \ubc0f \uadf8 \ud569\uae08) \uac00\uacf5\uc5d0 \uc801\ud569\ud569\ub2c8\ub2e4. \ub610\ud55c 300m\/min\uc758 \uace0\uc18d \uc808\uc0ad\ub3c4 \uac00\ub2a5\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">TiB\u2082\ub294 \uc721\uac01\ud615 \uacb0\uc815 \uc2dc\uc2a4\ud15c \uad6c\uc870\ub97c \uac00\uc9c0\uace0 \uc788\uc73c\uba70 \uc561\uccb4 \uc54c\ub8e8\ubbf8\ub284, \uad6c\ub9ac \ubc0f \uae30\ud0c0 \uae08\uc18d\uacfc\uc758 \uc811\ucd09\uac01\uc774 90 \u00b0 \uc774\uc0c1\uc774\uba70 1000 \u2103\uc5d0\uc11c \uc5ec\uc804\ud788 3.6 GPa\uc758 \uacbd\ub3c4\ub97c \uc720\uc9c0\ud569\ub2c8\ub2e4. TiB\u2082 \ucf54\ud305 \uc808\uc0ad \uacf5\uad6c\uc758 \ub9c8\ucc30 \uacc4\uc218\ub294 \uae30\uc874 \ucd08\uacbd\ud569\uae08\uc5d0 \ube44\ud574 40% \uc774\uc0c1 \uac10\uc18c\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">01 \ud2f0\ud0c0\ub284 \ud569\uae08 \uac00\uacf5\uc758 \ud2b9\uc131<\/h2>\n\n\n\n<ul class=\"wp-block-list\">\n<li>\ubc00\ub3c4\uac00 \uc791\uace0 \uc5f4\uc804\ub3c4\uc728\uc774 \ub0ae\uc73c\uba70 \uc808\uc0ad \uc2dc \uc808\uc0ad \uc5f4\uc774 \ud655\uc0b0\ub418\uae30 \uc27d\uc9c0 \uc54a\uace0 \uc808\uc0ad\ub0a0 \uadfc\ucc98\uc758 \uc791\uc740 \uc601\uc5ed\uc5d0 \uc9d1\uc911\ub418\uc5b4 \uacf5\uad6c \uc218\uba85\uc774 \ub9e4\uc6b0 \uc9e7\uc2b5\ub2c8\ub2e4. <\/li>\n\n\n\n<li>\ud2f0\ud0c0\ub284 \ud569\uae08\uc740 \ud654\ud559\uc801 \ud65c\uc131\ub3c4\uac00 \ub192\uace0 \uc11c\ub85c \uc811\ucd09\ud558\ub294 \uae08\uc18d\uacfc \uce5c\ud654\ub825\uc774 \ub192\uc544 \uacb0\ud569, \ud655\uc0b0 \uc99d\uac00, \uacf5\uad6c \ub9c8\ubaa8\ub97c \uc720\ubc1c\ud558\ub294 \uacbd\ud5a5\uc774 \uc788\uc2b5\ub2c8\ub2e4. <\/li>\n\n\n\n<li>\ud2f0\ud0c0\ub284 \ud569\uae08\uc758 \ub0ae\uc740 \ud0c4\uc131 \uacc4\uc218\uc640 \ub192\uc740 \ud0c4\uc131 \ubcc0\ud615\uc73c\ub85c \uc778\ud574 \uac00\uacf5\ub41c \ud45c\uba74\uc774 \ubc31 \ucee4\ud130 \ud45c\uba74\uacfc \ub113\uc740 \uc811\ucd09 \uba74\uc801\uc744 \uac00\uc9c0\uac8c \ub418\uc5b4 \ub9c8\ubaa8\uac00 \uc2ec\ud574\uc9c8 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/li>\n\n\n\n<li>\ud2f0\ud0c0\ub284 \ud569\uae08 \uc808\uc0ad \ubcc0\ud615 \uacc4\uc218\uac00 \uc791\uae30 \ub54c\ubb38\uc5d0 \uc2ac\ub77c\uc774\ub529 \ub9c8\ucc30 \uac70\ub9ac\uc758 \uc804\uba74\uc5d0 \uc788\ub294 \uce69\uc774 \uc99d\uac00\ud558\uc5ec \uacf5\uad6c \ub9c8\ubaa8\uac00 \uac00\uc18d\ud654\ub429\ub2c8\ub2e4. <\/li>\n<\/ul>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1280\" height=\"721\" src=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_04-1.jpg\" alt=\"\ud558\uc774\ud54c\uc2a4-\ud2f0\ud0c0\ub284 \ud569\uae08 \uc808\uc0ad \uacf5\uad6c \ucf54\ud305 \uae30\uc220 20231012_Page_04-1\" class=\"wp-image-5295\" srcset=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_04-1.jpg 1280w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_04-1-300x169.jpg 300w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_04-1-810x456.jpg 810w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_04-1-768x433.jpg 768w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_04-1-18x10.jpg 18w\" sizes=\"auto, (max-width: 1280px) 100vw, 1280px\" \/><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">\ud2f0\ud0c0\ub284 \ud569\uae08 \uc18c\uc7ac \uac00\uacf5 \uacf5\uc815 \uc808\uc0ad\ub825, \uace0\uc628, \ube60\ub978 \uacf5\uad6c \ub9c8\ubaa8, \uac00\uacf5 \uacf5\uc815 \uc2dc\uac04 \ubcc0\ud615 \ud5a5\uc0c1, \uc124\uacc4 \uc694\uad6c \uc0ac\ud56d\uc744 \ucda9\uc871\ud558\uae30 \uc704\ud574 \ubd80\ud488\uc758 \ud06c\uae30 \ubc0f \ubaa8\uc591 \uc815\ud655\ub3c4\ub97c \ubcf4\uc7a5\ud558\uc9c0\ub9cc \uacf5\uc791\ubb3c \ud45c\uba74\uc5d0 \uac00\uacf5 \ucee4\ud130 \ub9c8\ud06c, \ud504\ub9ac\uc998 \uc190\uc0c1, \ud45c\uba74 \ubbf8\uc138 \uade0\uc5f4, \uac00\uacf5 \uacbd\ud654, \uc870\uc9c1 \uc190\uc0c1 \ubc0f \uae30\ud0c0 \ud45c\uba74 \ubb34\uacb0\uc131 \ubb38\uc81c\uac00 \ub098\ud0c0\ub0a0 \uc218 \uc788\uc9c0\ub9cc \uac00\uacf5 \uacf5\uc815 \uc2dc\uac04 \ubcc0\ud615 \ud5a5\uc0c1.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1080\" height=\"607\" src=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u7528.jpg\" alt=\"\ud558\uc774\ud54c\uc2a4- \ud2f0\ud0c0\ub284 \ud569\uae08 \uc808\uc0ad \uacf5\uad6c \ucf54\ud305 \uae30\uc220\" class=\"wp-image-5297\" srcset=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u7528.jpg 1080w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u7528-300x169.jpg 300w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u7528-810x455.jpg 810w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u7528-768x432.jpg 768w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u7528-18x10.jpg 18w\" sizes=\"auto, (max-width: 1080px) 100vw, 1080px\" \/><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">02 \ud2f0\ud0c0\ub284 \ud569\uae08 \uac00\uacf5\uc758 \ubb38\uc81c\uc810<\/h2>\n\n\n\n<section class=\"wp-block-themepark-block-themepark-listbox thempark-block themepark_listbox shuang\" style=\"text-align:left;\"><ul class=\"themepark_listbox_list\" style=\"border-top:solid 1px #ccc; padding-top: 10px;padding-left:2%;padding-right:2%;\"><li style=\"font-size:20px;line-height:30px;margin-bottom:3px;padding-left:35px;\"><i class=\"fas fa-cog\" style=\"line-height:30px\"><\/i><span>CNC \ubc0f \uac00\uacf5 \ub9e4\uac1c\ubcc0\uc218<\/span><\/li><li style=\"font-size:20px;line-height:30px;margin-bottom:3px;padding-left:35px;\"><i class=\"fas fa-cog\" style=\"line-height:30px\"><\/i><span>\uc5e3\uc9c0 \uc900\ube44 \ubc0f \ucf54\ud305 \ud504\ub85c\uc138\uc2a4<\/span><\/li><li style=\"font-size:20px;line-height:30px;margin-bottom:3px;padding-left:35px;\"><i class=\"fas fa-cog\" style=\"line-height:30px\"><\/i><span>\uc0e4\ud504\ub2dd \uae30\uacc4 \ubc0f \ud504\ub85c\uc138\uc2a4<\/span><\/li><li style=\"font-size:20px;line-height:30px;margin-bottom:3px;padding-left:35px;\"><i class=\"fas fa-cog\" style=\"line-height:30px\"><\/i><span>\ub3c4\uad6c \uc7ac\ub8cc \uc120\ud0dd \ubc0f \ub3c4\uad6c \uc124\uacc4<\/span><\/li><\/ul><div class=\"themepark_listbox_ba\" style=\"opacity:1;\"><\/div><\/section>\n\n\n\n<h2 class=\"wp-block-heading\">03 CNC \uacf5\uad6c\uc5d0\uc11c PVD \ucf54\ud305\uc758 \uc5ed\ud560<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c \ud45c\uba74\uc758 \uacbd\ub3c4 \ud5a5\uc0c1, \uacf5\uad6c \ub0b4\ub9c8\ubaa8\uc131 \uac1c\uc120, \ub2e8\uc5f4 \ub610\ub294 \uc5f4 \uc804\ub3c4\uc131, \uc724\ud65c, \uc190\uc26c\uc6b4 \uce69 \uc81c\uac70.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub610\ud55c \ubd80\uc791\uc6a9, \uc608, PVD \ucf54\ud305\uc740 \uacf5\uad6c\uc5d0 \ubd80\uc791\uc6a9\uc744 \uc77c\uc73c\ucf1c \uc808\uc0ad\ub825\uc744 \ub5a8\uc5b4\ub728\ub9b4 \uc218 \uc788\uc2b5\ub2c8\ub2e4. PVD\uc5d0 \uc0ac\uc6a9\ub418\ub294 \uc7ac\ub8cc\uac00 \uac00\uacf5\uc758 \uc791\uc5c5 \uc870\uac74\uacfc \uc77c\uce58\ud558\uc9c0 \uc54a\uc73c\uba74 \ubbf8\ud06c\ub860 \ub450\uaed8\uc5d0\uc11c\ub3c4 \ubaa8\uc11c\ub9ac\uc5d0 \ubbf8\uce58\ub294 \uc601\ud5a5\uc774 \ud07d\ub2c8\ub2e4. \ub610\ud55c \uc811\ucc29\ub825\uc744 \ub192\uc774\uae30 \uc704\ud574 \uace0\uc628\uc5d0\uc11c \uacf5\uad6c \ucf54\ud305\uc744 \uc801\uc6a9\ud558\ub294 \uacbd\uc6b0\uac00 \ub9ce\uc740\ub370, \uc774\ub294 \ub0a0\uce74\ub85c\uc6b4 \ubaa8\uc11c\ub9ac\uc5d0\ub3c4 \uc0c1\ub2f9\ud55c \uc545\uc601\ud5a5\uc744 \ubbf8\uce69\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud558\uc774\ud54c\uc2a4 \ucf54\ud305 \uc7a5\ube44\ub85c \uc81c\uc870\ub41c TiB2 \ucf54\ud305\uc740 \ub2e4\uc74c\uacfc \uac19\uc740 \uc911\uc694\ud55c \uc7a5\uc810\uc774 \uc788\uc2b5\ub2c8\ub2e4.<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uac00\uacf5\ub418\ub294 \uc18c\uc7ac\ub294 \uc2dc\ud310\ub418\ub294 Ti6Al4V \ud2f0\ud0c0\ub284 \ud569\uae08 \uc18c\uc7ac\uc774\uba70, \ub3d9\uc77c\ud55c PVD \uc7a5\uce58\uc5d0\uc11c DCMS\uc640 Hipims\ub85c TiB2 \ucf54\ud305\uc744 \uc81c\uc870\ud558\uace0 \uad00\ub828 \uc808\ub2e8 \ud14c\uc2a4\ud2b8\ub97c \uc218\ud589\ud569\ub2c8\ub2e4. DCMS\uc640 Hipims\uc5d0\uc11c \ub3d9\uc2dc\uc5d0 \uc81c\uc870\ud55c TiB2 \ucf54\ud305\uc758 \uc131\ub2a5 \ucc28\uc774\ub97c \ube44\uad50\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1080\" height=\"607\" src=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims\u5236\u5907\u7684TiB2\u7ed3\u5408\u529b\u7ed3\u679c.jpg\" alt=\"Hipims\uc5d0\uc11c \uc900\ube44\ud55c TiB2 \uacb0\ud569 \uacb0\uacfc\" class=\"wp-image-5299\" srcset=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims\u5236\u5907\u7684TiB2\u7ed3\u5408\u529b\u7ed3\u679c.jpg 1080w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims\u5236\u5907\u7684TiB2\u7ed3\u5408\u529b\u7ed3\u679c-300x169.jpg 300w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims\u5236\u5907\u7684TiB2\u7ed3\u5408\u529b\u7ed3\u679c-810x455.jpg 810w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims\u5236\u5907\u7684TiB2\u7ed3\u5408\u529b\u7ed3\u679c-768x432.jpg 768w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims\u5236\u5907\u7684TiB2\u7ed3\u5408\u529b\u7ed3\u679c-18x10.jpg 18w\" sizes=\"auto, (max-width: 1080px) 100vw, 1080px\" \/><\/figure>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1080\" height=\"606\" src=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_15.jpg\" alt=\"\ud558\uc774\ud54c\uc2a4-\ud2f0\ud0c0\ub284 \ud569\uae08 \uc808\uc0ad \uacf5\uad6c \ucf54\ud305 \uae30\uc220 20231012_Page_15\" class=\"wp-image-5300\" srcset=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_15.jpg 1080w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_15-300x168.jpg 300w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_15-810x455.jpg 810w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_15-768x431.jpg 768w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_15-18x10.jpg 18w\" sizes=\"auto, (max-width: 1080px) 100vw, 1080px\" \/><\/figure>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1080\" height=\"607\" src=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_17-1.jpg\" alt=\"\ud558\uc774\ud54c\uc2a4-\ud2f0\ud0c0\ub284 \ud569\uae08 \uc808\uc0ad \uacf5\uad6c \ucf54\ud305 \uae30\uc220 20231012_Page_17-1\" class=\"wp-image-5301\" srcset=\"https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_17-1.jpg 1080w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_17-1-300x169.jpg 300w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_17-1-810x455.jpg 810w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_17-1-768x432.jpg 768w, https:\/\/www.naxauam.com\/wp-content\/uploads\/2023\/11\/Hipims-\u6280\u672f\u5728\u949b\u5408\u91d1\u5207\u524a\u5200\u5177\u6d82\u5c42\u4e2d\u7684\u5e94\u752820231012_\u9875\u9762_17-1-18x10.jpg 18w\" sizes=\"auto, (max-width: 1080px) 100vw, 1080px\" \/><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">\uc694\uc57d<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">TiB2 \ucf54\ud305\uc740 \ub192\uc740 \ud574\ub9ac\uc728 \ud2b9\uc131, \ub192\uc740 \uc5d0\ub108\uc9c0, \uc870\ubc00\ud558\uac8c \uc900\ube44\ub41c \ucf54\ud305, \ub0ae\uc740 \uc751\ub825 \ubc0f \uce58\ud551\uc774 \uc801\uc740 Hipims \uae30\uc220\uc744 \uc0ac\uc6a9\ud558\uc5ec \uc900\ube44\ub429\ub2c8\ub2e4. \ub3d9\uc2dc\uc5d0 B2O3 \uc561\ud654 \ud544\ub984\uc5d0 \uc758\ud574 \uc0dd\uc131 \ub41c TiB2 \ucf54\ud305 \uacf5\uad6c \ud45c\uba74 \uc0b0\ud654\ub294 \uc790\uccb4 \uc724\ud65c \ud6a8\uacfc\ub97c \ubc1c\ud718\ud558\uace0 \ub048\uc801 \ub048\uc801\ud55c \ub048\uc801\ud568\uc744 \uc904\uc785\ub2c8\ub2e4. \uc18c\ub7c9\uc758 \ub9c8\ubaa8\ub85c \ud2f0\ud0c0\ub284 \ud569\uae08 \uc808\uc0ad \uacf5\uad6c\uc758 \uc218\uba85\uc744 \ud6a8\uacfc\uc801\uc73c\ub85c \uc5f0\uc7a5 \ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table><tbody><tr><td>\ubaa8\ub378 \ubc88\ud638<\/td><td>\uc131\ubd84<\/td><td>\uacbd\ub3c4: HV<\/td><td>\ud544\ub984 \ub450\uaed8<\/td><td>\ud56d\uc0b0\ud654 \uc628\ub3c4<br>(\u00b0C)<\/td><td>\ub9c8\ucc30 \uacc4\uc218<\/td><td>\uc0c9\uc0c1<\/td><td>\uc801\uc6a9 \ubd84\uc57c<\/td><\/tr><tr><td>TiB2<\/td><td>TiB2<\/td><td>3000<\/td><td>1.0~3.0<\/td><td>600<\/td><td>0.3<\/td><td>\ubb34\ud654\uacfc \ubc18\ub3d9<\/td><td>\ube44\ucca0\uae08\uc18d \uac00\uacf5, \ud50c\ub77c\uc2a4\ud2f1 \uac00\uacf5<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uad00\ub828 \ub9c1\ud06c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"\/docs\/tib\u2082\u6d82\u5c42\u5728\u6709\u8272\u91d1\u5c5e\u52a0\u5de5\u9886\u57df\u7684\u5e94\u7528\/\">\ube44\ucca0\uae08\uc18d \uac00\uacf5\uc744 \uc704\ud55c TiB\u2082 \ucf54\ud305<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><\/p>","protected":false},"excerpt":{"rendered":"<p>TiB2\uff08\u4e8c\u787c\u5316\u949b\uff09\u6d82\u5c42 \u7eb3\u72eeTiB2\uff08\u4e8c\u787c\u5316\u949b\uff09\u6d82\u5c42\uff0c3000HV\u786c\u5ea6\uff0c\u91c7\u7528HiPiMS\u5236\u5907\uff0c\u5e94\u529b\u4f4e\uff0c\u6297\u5d29\u6027 [&hellip;]<\/p>","protected":false},"author":1,"featured_media":3169,"comment_status":"closed","ping_status":"closed","template":"","meta":{"themepark_post_bcolor":"#f5f5f5","themepark_post_width":"1022px","themepark_post_img":"","themepark_post_img_po":"left","themepark_post_img_re":false,"themepark_post_img_cover":false,"themepark_post_img_fixed":false,"themepark_post_hide_title":true,"themepark_post_main_b":"","themepark_post_main_p":100,"themepark_paddingblock":true,"footnotes":""},"doc_category":[138],"doc_tag":[264,265,266],"class_list":["post-3167","docs","type-docs","status-publish","has-post-thumbnail","hentry","doc_category-pvd","doc_tag-hipims","doc_tag-tib2","doc_tag-266"],"year_month":"2026-10","word_count":34,"total_views":"175","reactions":{"happy":"0","normal":"0","sad":"0"},"author_info":{"name":"\uc77c\uc885\uc758 \uc815\uc2e0","author_nicename":"lincy","author_url":"https:\/\/www.naxauam.com\/ko\/author\/lincy\/"},"doc_category_info":[{"term_name":"PVD\u5de5\u827a\u4e0e\u5e94\u7528","term_url":"https:\/\/www.naxauam.com\/ko\/\ubb38\uc11c-\uce74\ud14c\uace0\ub9ac\/pvd-\ud504\ub85c\uc138\uc2a4-\ubc0f-\uc801\uc6a9\/"}],"doc_tag_info":[{"term_name":"Hipims","term_url":"https:\/\/www.naxauam.com\/ko\/\ubb38\uc11c-\ud0dc\uadf8\/hipims\/"},{"term_name":"TiB2\u6d82\u5c42","term_url":"https:\/\/www.naxauam.com\/ko\/\ubb38\uc11c-\ud0dc\uadf8\/tib2-\ucf54\ud305\/"},{"term_name":"\u949b\u5408\u91d1","term_url":"https:\/\/www.naxauam.com\/ko\/\ubb38\uc11c-\ud0dc\uadf8\/\ud2f0\ud0c0\ub284\/"}],"_links":{"self":[{"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/docs\/3167","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/docs"}],"about":[{"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/types\/docs"}],"author":[{"embeddable":true,"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/comments?post=3167"}],"version-history":[{"count":8,"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/docs\/3167\/revisions"}],"predecessor-version":[{"id":5398,"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/docs\/3167\/revisions\/5398"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/media\/3169"}],"wp:attachment":[{"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/media?parent=3167"}],"wp:term":[{"taxonomy":"doc_category","embeddable":true,"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/doc_category?post=3167"},{"taxonomy":"doc_tag","embeddable":true,"href":"https:\/\/www.naxauam.com\/ko\/wp-json\/wp\/v2\/doc_tag?post=3167"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}